Carbide is the right answer for cutting and wear. It is the wrong answer for a 2,000°C furnace, a 0.03 mm filament or a radiation shield. That is where pure tungsten and its alloys come in.

Most of our enquiries arrive with the word "carbide" attached. Every so often one does not, and it is usually the more interesting job: a sapphire furnace that needs a crucible, a shielding wall for a medical accelerator, a filament drawn to 0.03 mm, a counterweight that has to fit in the same volume as a steel part but weigh twice as much.

These are tungsten products rather than cemented carbide. Same element, entirely different material behaviour, and a different set of rules for design and machining.

Pure tungsten: the high-temperature option

Commercially pure tungsten is 99.95% W, density 19.3 g/cm³, melting point 3,422°C. It keeps useful strength well above 1,500°C, which is why it appears in furnace furniture, evaporation boats, heating elements and sapphire crystal growth equipment.

Two things surprise first-time users. It is brittle at room temperature, so it cannot be bent or punched cold without cracking. And it oxidises in air above roughly 400°C, forming a volatile oxide that carries material away. In a vacuum or inert atmosphere it is stable; in open air at high temperature it simply disappears.

Heavy alloys: tungsten with a bit of give

Pure tungsten is hard to machine into complex shapes. Adding nickel, iron or copper produces a tungsten heavy alloy, typically 90–97% W by weight, with density from 17 to 18.5 g/cm³ and enough ductility to be turned, milled and drilled with carbide tooling.

Applications follow the density: counterweights for motorsport and aerospace, vibration damping masses, radiation shielding, ordnance components, and balancing weights where the envelope is fixed but the mass is not. A WNiFe alloy at 18 g/cm³ lets an engineer add 2.3 times the mass of a steel part without changing the mounting hole pattern.

The copper-bearing grades (WCu) trade some density for electrical and thermal conductivity. They are used for EDM electrodes, resistance welding tips and heat sinks in power electronics, where you need tungsten's thermal expansion matched to a ceramic and copper's conductivity to move heat out.

Wire: from 0.03 mm upward

Tungsten wire is drawn, not sintered to shape. It is sold by diameter, surface condition (black, cleaned, straightened) and temper. The fine end of the range, 0.03–0.1 mm, goes into filaments, thermocouples and medical devices. Thicker wire, 0.5–3 mm, is used for heating elements, electrodes and support pins in furnaces.

Handling fine wire is its own discipline. A 0.03 mm wire breaks under tension you would not notice by hand, and a kink cannot be straightened. If you are specifying it, ask about spool type and length per spool, because the packaging often decides whether the wire survives the process.

Sheet, plate and foil

Tungsten sheet is rolled and supplied annealed, from 0.05 mm foil up to 20 mm plate. Standard sizes are modest, typically 100 × 100 mm to 300 × 300 mm, because rolling wide tungsten sheet is difficult. Thickness tolerance tightens with size: expect ±10% on foil, ±0.05 mm on plate.

Typical uses are radiation shielding, sputtering targets, furnace reflectors, EDM electrodes for fine work, and backing plates where thermal expansion has to match a ceramic. For sapphire growth, tungsten crucibles and heaters are common because the melt is aggressive and the temperature is high enough to rule out most metals.

Design rules that save money

Five things, learned mostly from jobs that had to be remade:

  1. Keep wall thickness generous. Tungsten does not like thin sections. Below 1 mm, cracking during cooling or machining becomes likely.
  2. Avoid sharp internal corners. A fillet of at least 0.5 mm reduces cracking at the corner considerably.
  3. Design for the machining method. Tungsten is usually machined with carbide tooling at low speed, or with EDM. Grinding is preferred over turning for finish surfaces.
  4. Warm it before bending. Above 400°C, tungsten becomes workable. Below that, it snaps.
  5. Specify the atmosphere. If the part will run in air above 400°C, it needs a coating or a protective housing, and that should be in the design from the start.

Carbide or tungsten? A short decision path

If the part cuts, wears against abrasive material, or needs high hardness at room temperature, use cemented carbide. If it goes into a furnace above 1,200°C, needs density above 17 g/cm³, or must conduct heat and electricity while surviving high temperature, use tungsten or a tungsten alloy. If it needs to be machined into a complex shape and the temperature stays under 800°C, a heavy alloy is usually easier than pure tungsten.

We produce tungsten products in pure tungsten, WNiFe and WNiCu, plus wire, sheet, rod and crucibles, and we will say plainly when carbide is the better answer for an application. That happens more often than you might expect.

Molybdenum and tungsten are often quoted against each other for the same furnace part, and the molybdenum sheet, rod and wire guide covers the temperature and atmosphere limits where the cheaper material is the better one.

For a reference on size and form, this 0.03 mm tungsten filament wire shows the fine end of what we supply, and the 0.1–0.9 mm tungsten sheet listing covers thin rolled stock. Send the drawing, the operating temperature and the atmosphere through the quote form and we can usually confirm feasibility within a day.