Wear parts fail for different reasons, and a grade that survives abrasion will crack under impact. Sorting out which mechanism is eating your part is the whole job.
A quarry in Guangxi replaced the weld-on tips on their crusher hammers every three weeks. The maintenance team switched to a harder grade, which sounded sensible, and the tips started cracking within four days. Harder was the wrong direction. The tips were not wearing out; they were being destroyed by impact from oversize feed.
Carbide wear parts are usually selected by hardness, and that is the first mistake. Hardness resists abrasion. Toughness resists impact. The two move in opposite directions, and the only way to pick correctly is to know which one is actually killing the part.
Identify the mechanism first
Look at the failed part. The surface tells you what happened.
- Polished, smoothly worn areas with a measurable loss of section: abrasion. Fine particles sliding under pressure. This is the classic slurry, sand, cement and mineral handling case.
- Chipping, spalling, corners missing: impact. Something is hitting the part, or the part is hitting something.
- Craze cracks, heat checks, edge rounding without material loss: thermal cycling. Common in hot forming and in parts that see alternating hot and cold product.
- Pitting, discolouration, material missing around the binder: corrosion. Cobalt is the part that dissolves, so the carbide skeleton falls apart.
Mixed mechanisms are common. A chute liner in a wet mineral plant often sees abrasion plus corrosion, and the grade that fixes one may worsen the other.
Abrasion: lean on hardness and grain size
For pure abrasive wear, lower cobalt and finer grain give the longest life. A 6% cobalt grade at HRA 90.5–91.5 is the default. For very fine abrasive slurry, a sub-micron grade with 6% cobalt can outlast a coarser one by 30–50% because the mean free path between carbide grains is shorter, so the binder is better protected.
There is an exception. When the abrasive is coarse and the load is high (primary crusher liners, large chute plates), coarse grain with 8–10% cobalt often performs better, because a fine-grain grade chips at the surface and the chips become the start of larger fractures.
Impact: cobalt is your friend
Impact work needs 12–15% cobalt, medium grain, HRA 87–89. The higher binder content blunts crack tips and absorbs energy. If a part is cracking, this is the direction to move, even though the wear rate per hour will look worse on paper.
Geometry matters as much as grade. A sharp internal corner is a stress concentrator, and carbide will find it. A 1 mm radius at the root of a wear block can add more life than a grade change.
Heat: coarse grain and support
Thermal cycling cracks carbide because the surface expands faster than the core. Coarse grain resists crack propagation better than fine. Support matters too: a thin unsupported carbide plate in a hot application will crack regardless of grade, because the steel beneath it expands at a different rate.
For hot wear applications we usually recommend a brazed assembly with a compliant braze layer rather than a press fit, and a design that keeps the carbide in compression rather than tension.
Corrosion: less cobalt, higher density
In chemical or marine service, cobalt dissolves and leaves carbide grains unsupported. A 6% grade with high density and low porosity slows this down. For aggressive service, a nickel-bound grade is worth discussing, though it costs more and is not stocked everywhere.
Forms and how they are fitted
Wear parts come as plates, strips, blocks, tips, rods and custom profiles. The fixing method often decides the life:
| Form | Typical fixing | Watch out for |
|---|---|---|
| Weld-on tips | Brazed into a steel holder | Braze gap too thick causes cracking on cooling |
| Wear plates | Bolted or bonded | Bolt holes are stress risers; countersink generously |
| Wear strips | Brazed or clamped | Uneven clamping loads crack thin strip |
| Custom inserts | Press fit or shrunk into a case | Interference too high splits the case |
Brazing deserves its own note. The filler should be a silver-based alloy with a melting point well below the point where carbide is affected, and the gap should be 0.05–0.15 mm. A thick, lumpy braze joint is a crack waiting to happen, because the braze shrinks more than the carbide on cooling.
Cost per hour, not cost per kilogram
The right comparison is cost per operating hour. A $90 plate that lasts 400 hours costs less than a $60 plate that lasts 150 hours, even though the second one looks cheaper on the purchase order. We have seen plants switch to a lower-cost supplier and then quietly increase maintenance headcount to keep up with replacements.
Keep a simple record: part number, grade, hours in service, failure mode, and a photograph of the failed surface. After three or four replacements the pattern is obvious, and grade selection stops being guesswork.
Our carbide wear parts range covers weld-on tips, plates, strips, feed bowls and custom profiles, in grades from 6% to 15% cobalt. This weld-on tip for crusher hammers is a common starting point for impact applications, while the carbide plate for agricultural machinery suits abrasive sliding wear.
Wear plate that also has to hold an edge, such as a shear blade or a cutting strip, sits between this article and the blade edge geometry guide. If the part is a round section rather than a plate, the grade notes in the round bar article apply more directly.
If you can send a photo of the failed part along with the hours and the material being handled, we can usually recommend a grade and a geometry change in one pass. The contact form accepts images.